Engineering Excellence Across India, Africa & the Middle East

PET & Blow Moulding 8 min read

5 Common PET Preform Defects and How to Eliminate Them

PET preform defects are one of the most common sources of production loss in beverage packaging plants. Most defects are process-driven meaning they are preventable with the right parameter settings, material handling, and machine maintenance. Here are the five defects we see most often, and what causes them.

5 Common PET Preform Defects and How to Eliminate Them

Acetaldehyde (AA) content is the first concern for any food and beverage application. AA is a byproduct of PET degradation at high temperatures. The primary causes are excessive melt temperature, long residence time in the barrel, and poor drying. The fix is straightforward: dry your PET to below 50 ppm moisture, keep melt temperature within the material supplier's recommended range, and minimise residence time by matching shot size to machine capacity.

Crystallinity in the gate area — visible as a white, opaque spot at the injection point — is caused by slow cooling in the gate zone or excessive injection pressure. Check your gate cooling circuit for blockages or inadequate flow, and review your injection speed and pack pressure profiles. A well-cooled gate should be clear and amorphous.

Sink marks on the preform body are typically caused by insufficient pack pressure or pack time, or by a worn check ring that is allowing melt to flow back. Check your check ring for wear and verify that your pack pressure is being held for long enough to compensate for material shrinkage during cooling.

Black specks are a contamination issue — either from degraded material in the barrel, contaminated regrind, or a dirty hopper and drying system. The corrective action depends on the source: purge the barrel thoroughly, review your regrind quality and ratio, and inspect your material handling system for contamination points.

Wall thickness variation in the blown bottle — which often traces back to the preform — is caused by inconsistent cooling in the mould, uneven material distribution in the preform, or incorrect stretch-blow parameters. Measure preform wall thickness at multiple points around the circumference and along the length. Variation greater than 0.1 mm typically indicates a cooling or process issue that needs to be addressed before the blow moulding stage.

PET Preform Defect Analysis Process Optimisation Blow Moulding